A bimetallic screw barrel is not a coated barrel. It is a carbon steel barrel shell with a metallurgically bonded alloy liner on the bore, produced by centrifugal casting. The liner is what the melt actually touches, and it is chosen for the resin rather than for the price of the barrel. This article walks through the seven production steps, in the order they happen on the shop floor.
Why a bimetallic barrel instead of a nitrided one
A nitrided barrel is a single piece of steel with a hardened case. It is cost effective and works well for general purpose PE, PP and PS processing. But the case is thin, and once it is worn through there is no second life: the barrel is scrap.
A bimetallic barrel separates the two jobs. The outer shell carries the pressure, the flange, the feed throat and the heating elements, so it is made from a tough, inexpensive carbon steel. The bore carries the wear and the corrosion, so it is made from an alloy that would be far too expensive and too brittle to use for the whole barrel. That is why bimetallic barrels are the standard choice for glass fibre filled compounds, PVC, fluoropolymers, and any application where a nitrided barrel fails within a year.
Step 1 — Alloy selection
The alloy is selected from the resin and the filler, not from a catalogue page. Three questions decide it:
- What is the filler and how hard is it? Glass fibre, carbon fibre, mineral filler and ceramic powder each wear the bore differently. The harder the filler, the more carbide forming elements the liner needs.
- Is there chemical attack? PVC releases hydrogen chloride during processing, and some engineering resins carry acidic or halogenated additives. Here corrosion resistance matters more than raw hardness.
- What are the temperatures and pressures? High temperature accelerates both wear and corrosion, and it also sets the upper limit for the alloy.
Once the grade is fixed, the liner thickness follows the bore diameter and the expected service life. The selection is written on the drawing before any metal is cut, so the shop and the customer are working from the same document.
Step 2 — Preparing the steel shell
The barrel blank is bored oversize by exactly the liner thickness, so that after casting the bore comes back to the required dimension with enough stock left for finish grinding. The bore is then cleaned to bare metal: any oxide, oil or scale left on the surface becomes a bonding defect later. The shell is preheated before the alloy is introduced, which reduces the thermal shock at the interface.
Step 3 — Centrifugal casting
This is the step that decides the quality of the whole barrel. The shell is mounted in the casting machine and spun. The alloy is introduced into the rotating bore and heated until it melts. Centrifugal force throws the liquid alloy against the bore wall and holds it there while it solidifies.
Two things happen at once. First, the denser alloy is pressed outward, so gas porosity and low density inclusions are driven toward the inner surface where they can be machined away. Second, the liquid alloy is in intimate contact with the hot steel wall, which allows the two metals to diffuse into each other and form a real metallurgical bond rather than a mechanical one.
Spin speed, pouring temperature and shell preheat are set according to the bore diameter and the alloy grade. Get the preheat too low and the alloy chills before it can bond. Get the temperature too high and the interface grows a brittle intermetallic layer that cracks under thermal cycling.
Step 4 — Controlled solidification
Solidification is not left to the air. The barrel cools on a controlled curve so the alloy solidifies from the bore outward, which keeps shrinkage porosity away from the working surface. Slow enough cooling avoids cracks at the interface; fast enough cooling keeps the grain fine and the liner hard. This is where the interface is either sound or permanently weak, and it cannot be repaired afterwards.
Step 5 — Stress relief and rough machining
After casting, the barrel is stress relieved so that the machining that follows does not distort it. The bore is then rough bored and ground, leaving grinding stock. At this point the liner thickness is measured again: if the casting has run out of concentricity, it is caught here and not after finishing.
Step 6 — Finish machining
The bore is ground and honed to the final tolerance and surface finish, then the outside of the barrel is completed: flange facing and bolt pattern, feed throat opening, thermocouple holes, keyways and threads. The screw that runs inside it is machined to the matching clearance, because the barrel and screw are a pair and are normally supplied together.
Step 7 — Inspection before shipment
Every barrel leaves with a measurement record: bore diameter and taper, concentricity, liner thickness at both ends, liner hardness taken from a coupon of the same heat, and a bond check on the interface. Dimensions are checked against the customer drawing, not against a nominal table.
Bimetallic or nitrided — a quick rule of thumb
- Nitrided: unfilled PE, PP, PS, ABS; general purpose extrusion and injection; lowest cost; hardened case typically 0.45–0.7 mm with surface hardness around HV 900–1020.
- Bimetallic: glass or mineral filled compounds, PVC, engineering resins, high temperature melts, and any line where a nitrided barrel has already failed.
If you are not sure which one fits your material, send the resin datasheet and the machine model. The alloy recommendation should come from the material, and it costs nothing to check before the barrel is made instead of after.